How to Write a WPS and PQR: A Practical Guide with a Free Form Builder
Lay out a welding procedure specification and its PQR in ASME IX or ISO 15614 style, with joint sketch, pass table, arc energy and printable forms.

How to Write a WPS and PQR: A Practical Guide with a Free Form Builder
Any shop doing code welding on pressure equipment, piping or structures needs written procedures. A welding procedure specification tells the welder what to do; a procedure qualification record proves that doing it gives a sound weld. Keeping these documents tidy and consistent is a chore, and the free WPS and PQR Builder is meant to make the paperwork side easier. It lays out documents; it does not qualify procedures or certify that anything complies with a code.
WPS and PQR in a nutshell
The WPS gives ranges: a thickness range, a current range, a travel speed range, the positions allowed. The PQR records the single set of values actually used to weld a test coupon, and the results of testing it, typically tensile tests and bend tests, sometimes impact tests. A WPS lists the PQR or PQRs that support it, and the ranges in the WPS must stay within what those tests qualify under the code's rules.
Choosing a style
ASME Section IX has non-mandatory sample forms, QW-482 for the WPS and QW-483 for the PQR, and many companies follow their section order. ISO 15609-1 sets out what a WPS contains in ISO practice and ISO 15614-1 covers the qualification test. Choose either style and the labels change: P-numbers become material groups, process names become ISO 4063 numbers such as 111 for manual metal arc and 141 for TIG, and the printed headings follow.
Filling in the WPS
Work through the sections in order. Identification covers the company, WPS number, revision, date, the supporting PQR and the processes. The joint section takes the joint design, groove angle, root gap, root face and backing, and draws a sketch of the preparation that prints on the form. Base metals take the specifications, grades and groups, and the thickness and diameter ranges. Filler metals take the specification, classification, F-number and A-number or their ISO equivalents.
Positions, preheat and interpass temperature, post-weld heat treatment, shielding and backing gas, tungsten type and metal transfer mode, and technique notes such as stringer or weave beads and cleaning follow.
The pass table and arc energy
The electrical data is entered per layer: root, hot pass, fill and cap, with the process, filler and diameter, current type and polarity, and ranges of amperage, voltage and travel speed. For each row the builder works out the arc energy range, voltage times current times 60 divided by 1000 times travel speed in mm per minute. The low end uses the lowest current and voltage with the fastest travel; the high end the opposite. In ISO style the heat input also applies the process thermal efficiency factor.
Recording the PQR
On the PQR tab record the coupon material and thickness, filler, position, preheat and interpass temperature, PWHT, gas and the highest current, voltage and travel speed used. Add each tensile specimen's width, thickness and breaking load and the builder gives its tensile strength; add each bend specimen and its result.
A worked example
WPS-101 covers manual metal arc welding of SA-516 Grade 70 plate with E7018 electrodes in all positions, a 60 degree single V with a 3 mm gap. The root runs at 70 to 90 A, 20 to 23 V and 60 to 100 mm/min, which is 0.84 to 2.07 kJ/mm. PQR-101 used a 12 mm coupon at up to 175 A, 25 V and 110 mm/min, 2.39 kJ/mm. Its tensile specimens broke at 525 MPa in the base metal against a 485 MPa minimum, and four side bends passed.
Consistency checks
The checks tab compares the two documents and lists matches and mismatches: the thickness range against what the coupon qualifies, groups, filler numbers, processes, PWHT, preheat, arc energy when toughness was tested, tensile strength and bend results. The thickness range table is an editable example, written as simple expressions such as 2*T, so you can set it to the edition you work to. In the example a 12 mm coupon covers 5 to 24 mm and every check passes.
Printing and keeping records
Print the WPS and PQR as separate forms with signature lines. Save each pair as a named project, and export it as JSON to back it up or share it.
The important caveat
Codes list essential, supplementary essential and non-essential variables, with detailed rules on what each test qualifies. The builder does not contain those rules, and a printed form is not a qualified procedure. Real test welds, testing by a competent laboratory and approval by the responsible welding engineer or inspector are what make a procedure valid.